Melting Points of Polymers
Polymer Name |
Tm1 (K) |
Poly(acrylonitrile), syndiotactic | 594 |
Poly(6-aminocaproic acid) | 497 |
Poly(trans-butadiene), 90% trans - 7% vinyl | 320, 361 |
Poly(1-butene), isotactic | 398 |
Poly(caprolactam) | 495 |
Poly(decamethylene adipamide), Nylon 10,6 | 508 |
Poly(decamethylene sebacamide), Nylon 10,10 | 475 |
Poly(etheretherketone), PEEK | 630 |
Poly(ethylene adipate) | 336 |
Poly(ethylene oxide), PEG | 339 |
Poly(ethylene terephthalate), PET | 537 |
Poly(ethylene) | 414 |
Poly(hexamethylene adipamide), Nylon 6,6 | 545 |
Poly(hexamethylene sebacamide), Nylon 6,10 | 497 |
Poly(hexamethylene suberamide), Nylon 6,8 | 509 |
Poly(methyl methacrylate), isotactic | 417 |
Poly(methyl methacrylate), syndiotactic | 473 |
Poly(methylene oxide), POM | 445 |
Poly(4-methylpentene) | 516 |
Poly(propylene), isotactic | 452 |
Poly(styrene), isotactic | 515 |
Poly(styrene), syndiotactic | 549 |
Poly(tetramethylene oxide), PTMO | 314, 333 |
Poly(trans-1,4-butadiene) | 371, 417 |
Poly(vinyl alcohol) | 504, 539 |
Poly(vinyl chloride), PVC | 493, 578 |
Poly(vinyl fluoride) | 472 |
Poly(vinylidene chloride) | 468 |
Poly(vinylidene fluoride) | 450 |
Poly(ω-undecanamide), Nylon 11 | 460 |